Advanced packaging

Dual Damascene in Advanced Packaging: Hybrid-Bonding Pads, Fine-Pitch RDL, and Bridge Dies

Published · Last checked

Quick answer

Dual damascene is the way copper wiring has been made on chips since the late 1990s: trenches and vias are etched into the dielectric first, lined with a barrier and a thin copper seed, filled by electroplating, and the excess copper is polished away so that the wiring ends up inlaid in the insulator [D1]. The step that made it work is "superfilling", plating that deposits faster inside a feature than on the field around it; IBM's account dates its discovery to as early as 1990, and a NIST model later explained it by an accelerating additive that becomes more concentrated on concave surfaces as they shrink [D1][D2]. In packaging, the sources read for this page document the process in two places. One is the copper pads that hybrid bonding joins: a flow reported from Applied Materials exposes the pads by etching, then deposits, plates and polishes, and the report says a dishing depth below 5 nm was needed for bonding yields above 70% in that work [D7]. The other is fine redistribution wiring: TSMC has published a demonstration of two layers of dual-damascene copper RDL at 2 µm lines and 1 µm spaces, with a polishing step [D9]. For silicon interposers and bridge dies, the sources read here describe the wiring but not how it is made [D4][D5]; that it is damascene is this page's inference [interpretation].

What this page does not cover: the general theory of chip back-end wiring (BEOL) beyond what packaging borrows from it; how to calculate plating thickness or time, which the Copper Electroplating Guide covers and which, as explained below, does not predict feature fill; and how bridges and interposers are used architecturally (Chiplets Explained, Intel EMIB Explained).

Status vocabulary used on this page: announced, demonstrated, pilot production, volume production; every status is dated to its source.

Why it exists and how it works

Why copper, and why inlaid. Copper replaced aluminum in chip wiring because it cuts wire resistance by up to about 45% and resists electromigration far better; IBM's early tests showed a median lifetime more than a hundred times longer for copper lines than for titanium-clad aluminum at the same stress [D1]. But there was no workable equivalent, for copper, of the blanket deposition and reactive-ion etch used to pattern aluminum, so the wiring geometry was inverted: the insulator is etched into the shape of the wiring, and copper is deposited into it [D1]. In dual damascene the via and the trench above it are metallized and planarized together, so a wiring level and its connection downward are completed in the same deposition and polish [D1].

The process. The sequence has five steps: pattern and etch the via and trench into the dielectric; deposit a thin barrier that stops copper diffusing into the insulator; deposit a copper seed layer so the whole surface conducts; electroplate copper until the features are filled and an "overburden" covers the field; and polish the overburden off by chemical-mechanical planarization (CMP) until only the inlaid copper remains [D1]. The account cited here describes these as operations on chip wafers [D1]. TSMC's RDL demonstration was likewise made on 300 mm wafers [D9].

1. Etch via and trench 2. Barrier, seed thin lines 3. Plate bottom-up, overburden 4. CMP Cu inlaid, flush 5. Next level starts on top Dielectric Copper Barrier Seed Growth front Barrier and seed are drawn as thin lines, not to scale.
Figure 1. One dual damascene level in five frames: (1) the via and the trench above it etched into the dielectric, the via landing on copper in the level below; (2) a barrier and a copper seed lining the opening; (3) electroplated copper filling the via and trench from the bottom up, with an overburden over the field, the dashed lines marking earlier growth fronts; (4) after chemical-mechanical planarization, copper inlaid and flush with the dielectric; (5) the next level starting on top [D1][D2]. Drawing choices: the via is 1 unit wide and 1 deep, the trench 1.5 units wide and 1 deep, the overburden 0.5 unit; the growth fronts are schematic; the barrier and seed are drawn as thin lines, not to scale.

Superfilling. If copper plated at the same rate everywhere in a feature, the result would be a seam where the sidewalls meet, or a void in a feature that is narrower at the top than below [D1]. Superfilling avoids both because the deposition rate inside the feature exceeds the rate on the field [D1]. IBM's 1999 account reasons as follows: the metal seed connects the whole surface electrically, the ohmic drop in the electrolyte is small across a feature of this size, and, assuming further that differences in copper-ion concentration are small, the account attributes the difference in plating rate between two points to the additives; it notes that the assumption weakens as aspect ratio rises and features shrink [D1]. NIST's curvature-enhanced accelerator coverage (CEAC) model made the idea quantitative: an accelerating additive adsorbed on the surface becomes more concentrated where the surface is concave and shrinking, as at the bottom of a filling trench, and more dilute on convex corners that grow, and the model's predictions agree with feature-filling experiments [D2]. In the additive system NIST studied, the accelerator is the additive known as SPS, with chloride, and the suppressor is polyethylene glycol (PEG) with chloride; its surface study found the SPS–chloride phase displacing the inhibiting PEG–chloride layer and preventing it from forming [D3]. The same literature describes two- and three-component additive systems [D2]. This page describes the mechanism only and reports no maker's bath composition or operating window.

1. Seeded trench accelerator spread over the surface 2. Bottom filling the bottom shrinks, accelerator crowds 14 accelerator dots in each frame; no concentrations implied. accelerator (SPS) suppressor (PEG–Cl) Copper Dielectric
Figure 2. The curvature-enhanced accelerator coverage (CEAC) idea in one trench, before filling and while the bottom fills [D2]. The accelerator (SPS) sits on the surface alongside the suppressor (PEG–Cl) film [D3]; as the bottom fills, its area shrinks and the same accelerator crowds onto it, so the bottom plates faster, while the dots on the corners and the field spread out [D2]. Both frames carry the same 14 dots, a drawing choice that stands for the model's simplification that adsorbed accelerator is conserved as the area changes. No concentrations are implied; schematic.

Why Faraday's law is not enough here. Faraday's law gives the mass of copper deposited for a given charge; on a flat surface, once the plated area and the current efficiency are known, that fixes the average thickness, which is the calculation the Copper Electroplating Guide walks through [D8]. Inside a damascene feature the same charge can produce a void-free fill or a seamed one, and the law cannot tell which: fill quality depends on where the copper goes, which is the subject of the superfilling work above, not on how much copper there is [D1][D2]. In this page's interpretation, a thickness calculation is a starting estimate for the copper deposited over the field; it says nothing about whether the via underneath is sound, or about local thickness and uniformity [interpretation].

Where it is used in packaging

Interposers and bridge dies. TSMC describes the silicon interposer of CoWoS-S as providing high-density interconnects, and a published example of an Intel embedded bridge has four metal layers at 2 µm line and space [D4][D5]. Neither source says how that wiring is made. That it is damascene is this page's inference from the fact that copper wiring on chips has been made that way since the late 1990s [D1][interpretation]. Through-silicon vias are covered in TSV vs TGV; the IBM account read for this page compares its sub-micrometer features with through-hole plating, not with through-silicon vias, so this page draws no conclusion about via filling at that scale from it [D1].

Fine-pitch RDL. Packaging wiring can also be made by plating through a resist mask: a seed layer is deposited first, copper is plated only where the mask leaves the seed exposed, and the seed is removed afterward [D1]. A 2020 conference paper on panel-level packaging describes electrolytic copper pattern plating in a photoresist pattern and assigns the RDL layers of its example to the modified semi-additive process (mSAP) [D10]. TSMC's CoWoS-R, an RDL interposer of polymer and copper traces, has a minimum line width and spacing of 2 µm; the CoWoS page does not say how the traces are formed [D4]. Damascene RDL is also documented: a TSMC research abstract from 2018 describes two layers of embedded copper dual-damascene RDL at 2 µm lines and 1 µm spaces on 300 mm wafers, with a CMP step [D9]. That is a published demonstration. This page does not read it as the process of any product, and the sources read here do not say where any maker changes from one process to the other [interpretation].

Hybrid-bonding pads. Hybrid bonding joins two surfaces that are each a mosaic of dielectric and copper pads, with no solder; Hybrid Bonding vs Microbumps describes the joint [D8]. Intel's brief describes Foveros Direct 3D as direct copper-to-copper hybrid bonding at sub-10 µm pitch with up to ten times the interconnect density of microbumps, presents it as available on Intel Foundry process nodes, and does not state a production status [D6]. A pad flow reported from Applied Materials at ECTC 2022 exposes the last-level pads by etching, then applies physical vapor deposition, electrochemical deposition and CMP before dielectric bonding and annealing [D7]. This page reads that sequence as a damascene sequence, though the report does not use the word [interpretation]. The same report says that in Applied Materials' work a dishing depth below 5 nm was needed for bonding yields above 70% at a bonding temperature of 350 °C, a result for that work's conditions rather than a general rule, and that SK hynix's paper at the same conference kept copper dishing below 5 nm on both wafers of a wafer-to-wafer flow whose wafer yields were reported as the same as its production DRAM [D7]. Inlay and polish is not the only route: Hybrid Bonding vs Microbumps records a polymer-dielectric structure bonded at about 180 °C without CMP [D8].

Before anneal Gap remains over the pads After anneal Cu expanded, gap closed Silicon die Dielectric Inlaid Cu pad 9 µm pitch: one frame 2 µm
Figure 3. A hybrid-bond interface before and after anneal: two dies face to face, each with inlaid copper pads recessed below the dielectric. Before anneal the dielectric surfaces are in contact with a gap over the pads; after anneal the dielectric is bonded and the copper has expanded to close the gap [D8]. Drawing values: the 9 µm pitch is the SoIC-X entry for 2022–2023 on TSMC's 2024 roadmap as reported, cited in Hybrid Bonding vs Microbumps, a dated roadmap figure rather than a product status [D8]; the 4 µm pad width is a drawing choice; the 5 nm recess is drawn at the dishing limit reported for the Applied Materials test structures, where the reported condition was below 5 nm, and is exaggerated about 100 times [D7]. The drawing is a composite, not one measured structure.

Alternatives and trade-offs

Table 1. Semi-additive plating and dual damascene compared.
Semi-additive (pattern plating through resist)Dual damascene (plate into etched dielectric, then CMP)
Where the pattern is definedIn the openings of the resist mask [D1]In the etched dielectric; the polish reveals the pattern [D1]
Packaging examples in the sources readRDL layers in a panel-level packaging example, by mSAP [D10]; CoWoS-R reaches 2 µm line and space, process not stated on the CoWoS page [D4]Hybrid-bonding pads in a reported Applied Materials flow [D7]; a TSMC demonstration of RDL at 2 µm lines and 1 µm spaces [D9]; silicon interposers and bridge dies by this page's inference only [D4][D5]
Fill requirementCopper plates only where the mask leaves the seed exposed [D1]Each feature is a recess to be filled without a void or seam, which is what superfilling addresses [D1][D2]
Planarity—Set by CMP; dishing below 5 nm in the hybrid-pad work cited [D7]
EquipmentPanel plating equipment in the panel-level example [D10]Etch, barrier and seed deposition, plating and CMP on wafers in the account cited [D1]

Engineering interpretation, and what is uncertain

The following is interpretation drawn only from the sources above.

In the sources read for this page, the best-documented packaging use of an inlay-and-polish sequence is the hybrid-bonding pad, and what the report cited here describes is the pad surface: dishing in nanometers and, separately, a requirement for sub-nanometer surface roughness [D7]. This page's reading is that the polish, and not only the fine geometry, is part of what the process brings to packaging; the sources do not compare the two, and a polymer structure bonded without CMP shows that polishing is not the only way to prepare a bonding surface [D8].

What limits superfilling changes with scale. IBM's account builds its argument for sub-micrometer features on assumptions that it says weaken as aspect ratio rises and features shrink, and it notes that for deeper features, with an example in excess of 50 µm, the ohmic drop in the electrolyte may no longer be negligible [D1]. This page's reading is that a fill established for one feature size and aspect ratio has to be re-established for another.

Faraday's law and superfilling answer different questions. The first says how much copper a given charge deposits; the second concerns whether the copper went where it was needed. A thickness calculation of the kind in the Copper Electroplating Guide is a starting point for a damascene process, not a description of the fill.

Uncertain: the sources read for this page do not say where any maker changes RDL from pattern plating to damascene and give no production dishing specifications or CMP recipes; the additive description here is the generic one in the public literature. Two sources were read only as abstracts, the 1998 IBM paper and the NIST surface study, so the statements drawn from them are limited to what the abstracts and the 1999 IBM article support.

Further reading and sources

On this site: the Copper Electroplating Guide for Faraday's law and current-density units; the Plating rate calibration guide for fitting measured thickness against time; Panel-Level Packaging Explained for RDL on panels; Chiplets Explained and Intel EMIB Explained for the interposers and bridges discussed above; Hybrid Bonding vs Microbumps for the joint the inlaid pads form; Packaging Substrates and Interposers for the materials these parts are built on; TSV vs TGV for through-silicon vias.

Sources (grade A unless noted):