Advanced packaging

TSV vs TGV: Vertical Vias Through Silicon and Through Glass

Published · Last checked

Quick answer

A through-silicon via (TSV) and a through-glass via (TGV) do the same job: each carries a signal or power vertically through a carrier so that something can sit on top of something else. They differ in the material they pass through and, in the sources read for this page, in how the hole is made and in what the published work is concerned about [interpretation]. A TSV is a copper-filled hole through a silicon die or interposer; the test structures in the review cited here are 5 µm in diameter by 50 µm deep and 10 µm by 100 µm, and the concerns it documents come from copper and silicon expanding differently with temperature (about 17 against about 2.3 ppm per °C in its model): stress around the via, the copper "pumping" out of the via top during thermal cycling, and a keep-out zone that the stress imposes on nearby transistors [T1]. A TGV is a hole through a glass panel or wafer. Corning's published capability, from 2015–2016, is 25–100 µm in diameter at a minimum pitch of about twice the diameter, in panels up to 515 × 515 mm; a trade-press article on LPKF's laser-and-etch process carries the company's claim of structures below 5 µm [T2][T3]. Glass is an insulator, so the via needs no insulating oxide liner (a barrier or adhesion layer under the copper is a separate matter), and in Corning's transmission-line tests glass lost less signal than standard silicon above a few hundred MHz; Corning's papers also treat the handling of thin glass as a problem to be solved, and its vias of about 30 µm in 100 µm glass were demonstrated on 150 mm wafers [T2]. This page's reading is that the choice between the two follows from the choice of carrier, silicon or glass, which is the subject of Packaging Substrates and Interposers [interpretation].

What this page does not cover: the material comparison of silicon and glass as substrates (Packaging Substrates and Interposers), the copper fill mechanism itself (Dual Damascene in Advanced Packaging), and the bonding that stacks dies once the vias exist (Hybrid Bonding vs Microbumps).

Status vocabulary used on this page: announced, demonstrated, pilot production, volume production; every status is dated to its source.

Why they exist and how they work

The TSV. Stacking dies, or putting dies on a silicon interposer, needs a vertical path through silicon [T1][T6]. The TSV is that path. The process steps named in the review cited here are a deep etch into the wafer, the deposition of barrier and seed layers, and copper electroplating [T1]. A TSV also has an insulating liner between the copper and the silicon, since silicon conducts [definition]. In a via-middle sequence the vias are made after the transistors but before the back-end wiring; in via-last they are made after the wiring [T1]. HBM Explained describes the later step in which the dies are thinned so that the vias can be exposed from the back [T7]. The test structures the review reports are 5 µm × 50 µm and 10 µm × 100 µm (diameter × depth), and its stress analysis compares an aspect ratio of 10 on a thick wafer with an aspect ratio of about 2 on a thin wafer [T1].

The physics that follows is thermal. The review's model takes copper at about 17 ppm per °C and silicon at about 2.3 ppm per °C; on heating the copper is put into compression and on cooling into tension, and the driving force for delamination at the interface on cooling is about twice that on heating [T1]. For a 10 µm via cooled by 250 °C, the modeled steady-state energy release rate is 6–7 J/m², which the review sets beside the adhesion energies of the copper–silicon and copper–oxide interfaces and the cohesive energy of silicon [T1]. Two consequences matter to the designer. Copper can extrude from the via top and stay extruded after cooling: the review reports average extrusions of 117 nm for small-grain and 147 nm for large-grain copper in 5.5 µm × 55 µm vias, and describes post-plating anneals at 375–420 °C, typically for 20 minutes, to stabilize the grain structure [T1]. And the stress field shifts carrier mobility in the surrounding silicon, so transistors are kept out of a zone around each via: 4 µm or less for the 5–10 µm vias tabulated in the review, and about 2 µm for a 7 µm via-last via under a 1% ring-oscillator frequency criterion, with finite-element models over-predicting the zone for vias of 10 µm or smaller [T1].

TSV after thinning Cu extrusion at the top (not to scale) Transistors Keep-out zone, no transistors Oxide liner and barrier (not to scale) Expansion on heating Thinned silicon Back-side reveal Cu via 10 µm
Figure 1. A copper through-silicon via after the wafer has been thinned to reveal the via from the back. On heating, the copper expands more than the silicon around it (side arrows) and can extrude from the via top (upward arrow); transistors are kept out of a zone around the via at the transistor level [T1]. Cited values: a 10 µm via, from a 10 µm × 100 µm test structure, and a keep-out zone of 4 µm on each side, the upper bound tabulated for 5–10 µm vias [T1]. Drawing choices: about 20 µm of silicon, an aspect ratio of about 2 applied to that diameter; the oxide liner, barrier and extrusion are not to scale. The values are assembled from the cited literature, not taken from one measured structure. Red marks expansion and the keep-out zone; the color indicates function, not material.

The TGV. Glass is an insulator, so a through-glass via needs no insulating liner between the copper and the glass [T2]. Corning's papers do not say how its vias are formed; the two other sources read for this page describe laser-based routes [T3][T4]. Corning's published capability, as of 2015–2016, covers fusion-formed glass panels up to 515 × 515 mm and wafers up to 300 mm, 0.1–0.7 mm thick, with vias of 25–100 µm outer diameter at a minimum pitch of about twice the diameter; its test vehicles include 35 × 125 µm blind vias and vias of about 30 µm in 100 µm glass, the latter demonstrated on 150 mm wafers [T2]. LPKF's laser-induced deep etching (LIDE), as described in a trade-press article, uses a single laser pulse to modify the glass through its entire thickness along the via, then a wet etch that removes the modified glass much more rapidly than the rest; the article carries the company's claims of an aspect ratio written as >1:10, structures below 5 µm and no micro-cracks (vendor claims as reported) [T3]. A Georgia Tech Packaging Research Center presentation from November 2019 lists microvias of 5 µm diameter at 10 µm pitch made with a picosecond ultraviolet laser, and through-glass vias below 100 µm made with a femtosecond laser [T4]. Corning's glasses span a CTE (coefficient of thermal expansion) range of about 3 to 9 ppm per °C [T2]. In Corning's thermal-cycling test, eight arrays from each type of glass, chosen as known-good and of 400 vias each, showed 100% yield after 1,000 cycles from −40 to 125 °C, and the median chain resistance on the low-CTE glass rose from about 10 to about 17 Ω [T2]. That is a result for pre-selected arrays, not a manufacturing yield [interpretation].

TGV and TSV at the same scale TSV, 10 µm (Figure 1) Glass, 100 µm Cu-filled TGV, 30 µm No oxide liner 10 µm LIDE, vendor-described (inset, not to scale) 1. Laser modification 2. Wet etch opens the via
Figure 2. A copper-filled through-glass via at the same scale as Figure 1: glass 100 µm thick with a via about 30 µm across, the dimensions of a Corning test vehicle [T2]. Glass is an insulator, so the via has no oxide liner [T2]. The outline at the left is the 10 µm TSV of Figure 1 at the same scale, for comparison. Drawing choices: the straight via walls, the width of glass shown and the TSV outline. Inset, not to scale: the laser-induced deep etching (LIDE) route as the vendor describes it in a trade-press article, a laser modification line through the glass followed by a wet etch that opens the via [T3].

Where they are used

By application and dated. HBM stacks (high-bandwidth memory, stacked DRAM): the JEDEC HBM3 standard, announced in January 2022, supports 4-, 8- and 12-high TSV stacks with provision for a future extension to 16-high, with 16 channels, up to 6.4 Gb/s and up to 819 GB/s per device [T5]; a published standard is not a product status. SK hynix said in September 2024 that it had begun mass production of a 12-layer HBM3E product, as recorded in HBM Explained [T7]. Silicon interposers: TSVs are the vertical path through the silicon interposer of TSMC's CoWoS-S, which TSMC's CoWoS page, accessed November 2026, says has been in production since 2012 [T6]. Bridges: Intel's July 2025 brief says TSVs have been added to EMIB-T and does not state volume production of EMIB-T; Intel EMIB Explained records a later company statement of a target to support customer ramps in 2027 [T6][T7]. How the stacked dies are then joined is covered in Hybrid Bonding vs Microbumps.

Announced and demonstrated. Corning's and Georgia Tech's results are demonstrations on test vehicles [T2][T4]. TGVs belong to the glass-core substrate and glass interposer programs described in Packaging Substrates and Interposers, and the dated company statuses are kept on that page: in its reading, Samsung Electro-Mechanics is at pilot production of prototypes, Absolics is at demonstrated with samples, and LG Innotek and Intel are at announced, and none of the statements read for it, dated 2023 to October 2026, claims volume production [T7]. This page adds no status of its own for TGVs.

Alternatives and trade-offs

Table 1. Through-silicon vias and through-glass vias compared.
TSVTGV
CarrierSilicon die or interposer; CTE about 2.3 ppm per °C in the review's model [T1]Glass panel or wafer; CTE range about 3–9 ppm per °C across Corning's glasses [T2]
Diameter × depth in the cited work5 µm × 50 µm and 10 µm × 100 µm test structures [T1]25–100 µm diameter in 0.1–0.7 mm glass, Corning's 2015–2016 capability [T2]; structures below 5 µm claimed for LIDE (vendor claim as reported) [T3]
Pitch or keep-out zoneKeep-out zone of 4 µm or less for the 5–10 µm vias tabulated [T1]Minimum pitch about 2× the via diameter [T2]; 10 µm pitch for 5 µm laser-drilled microvias [T4]
How the hole is madeDeep etch, barrier and seed layers, copper electroplating [T1]Not stated in Corning's papers [T2]; laser modification plus wet etch (LIDE, vendor claim as reported) [T3]; picosecond and femtosecond laser drilling [T4]
ElectricalStandard silicon lost more signal than glass above a few hundred MHz in Corning's transmission-line tests [T2]Insulator; low or adjustable dielectric constant, in Corning's description [T2]
Thermal and mechanical concernsCopper–silicon expansion mismatch: extrusion, delamination, keep-out zone [T1]Thin-glass handling and bonding planarity in Corning's demonstrations [T2]; the vendor claims no micro-cracks for LIDE [T3]
FormatSilicon wafers in the cited test structures [T1]Panels up to 515 × 515 mm and wafers up to 300 mm [T2]
Status (dated)Volume production: 12-layer HBM3E (SK hynix statement, September 2024) and CoWoS-S (TSMC page, accessed November 2026); EMIB-T: TSVs added per Intel's July 2025 brief, with a 2027 customer-ramp target stated later [T6][T7]Demonstrated on test vehicles (Corning 2015–2016, Georgia Tech 2019) [T2][T4]; for company programs see Packaging Substrates and Interposers, where none of the statements read claims volume production [T7]

Engineering interpretation, and what is uncertain

The following is interpretation drawn only from the sources above.

The TSV concerns in the review share a root: copper in a hole in a material that expands much less than it does. Extrusion, delamination and the keep-out zone all trace back to that mismatch in the review's account [T1]. The review treats grain-stabilizing anneals, via size and aspect ratio separately, and notes that smaller vias do not necessarily improve the largest extrusions or reliability [T1]. This page's reading is that a TSV design is a thermal-mechanical design as much as an electrical one.

The TGV sources raise different concerns. Because glass is an insulator the liner is not needed, and because the glass CTE can be chosen, Corning discusses it as a way to manage the warpage of a stack [T2]. What the Corning papers return to is handling: the carrier, the thinness of the glass and the planarity of the bond in its demonstrator [T2]. Corning's thermal-cycling test still inspected the vias themselves for cracking and delamination, so the sources do not show that via-level failure has gone away [T2].

The size gap in the cited work is large: test-structure TSVs of 5–10 µm against a published TGV capability of 25–100 µm [T1][T2]. That is a comparison of what these particular sources report, not a rule about where each via can be used; TSVs appear in dies, interposers and bridges on this page alone. LPKF's claim of structures below 5 µm is a vendor claim about structures, not a stated diameter or pitch for copper-filled vias, and it is the figure to check against later sources [T3].

Uncertain: the sources used here give no TGV diameters or pitches for a named production product; LPKF's sub-5 µm and crack-free claims are the vendor's; the Georgia Tech figures come from a research-center presentation that mixes results with targets; keep-out-zone values depend on via diameter, process sequence and transistor type, and the cited numbers are for the specific test structures named.

Further reading and sources

On this site: Packaging Substrates and Interposers for the silicon and glass carriers these vias pass through; Dual Damascene in Advanced Packaging for how the copper gets into the via; Hybrid Bonding vs Microbumps for how the stacked dies are joined.

Sources (grade A unless noted):